Dacromet is a trademark. I end up saying that about twice a month, usually to somebody who has a drawing that says "Dacromet or equivalent" and a supplier who has told him the equivalent is whatever grey coating is in the barrel that week.
The generic name is zinc-aluminium flake coating. Zinc and aluminium platelets in an inorganic binder, cured somewhere around 300 degrees C, film weight 8 to 12 microns for a single coat, roughly double that for two. That last clause is where most of the trouble lives.
The name is a trademark, which is the first problem
Ask for coating weight in grams per square metre. Not the brand. A 240 g/m² single coat and a 480 g/m² double coat are different products, and both arrive with the same word on the box.
What you get for the weight: no hydrogen in the process, so no delayed brittle failure on high-strength steel, which is why the coating shows up on property class 10.9 and above where electroplating is a genuine risk. Barrier plus sacrificial protection at a scratch - the zinc gives itself up before the steel does, which is what separates this from paint.
What you don't get is abrasion resistance. Ten microns doesn't survive being dragged across a slab or driven through a steel hanger or spun under an oversized washer. Those are handling events, they happen before the screw is in the timber, and on a deck the resulting bare patch sits under a board in permanent damp.
Eighty millimetres, minus the board
The 80 is overall length under the head. Load is carried by thread engagement, which is 80 minus board thickness minus washer, plus or minus the unthreaded shoulder.
Twenty-five millimetre board over a joist leaves about 52 mm of thread. Thirty-two leaves 45. Thirty-eight leaves 39. Forty-five leaves 32.
Run those through the Eurocode 5 withdrawal expression with a characteristic density of 350 kg/m³ and the capacity goes 6.5, 5.5, 4.8, 4.0 kilonewtons as the board gets thicker. Indicative numbers, and not a substitute for the ETA that should be in the box, but the shape of the curve is the point: the same part number loses roughly 40 percent of its grip because somebody chose a thicker deck board.
Nobody runs that calculation. Two decks both specified as "M8x80" end up performing like different products, and the paperwork says they're identical.
The structural screw that isn't a decking screw
A structural screw is replacing a bolt, a hanger, or a connector, and has to be qualified as one. Longer unthreaded shoulder, so the two members pull tight before the thread bites the second one. Thicker shank relative to thread. Washer head, or hex with a separate plate. And a code report with a number on it.
A wafer-head decking screw with full-length thread is a perfectly good product. In a structural position it can't clamp, it puts thread in the gap between the members where thread does nothing, and it has no published capacity.
Inspectors ask for the paper. The paper is the difference, which is a strange thing to say about two objects that look nearly the same in the hand.
Treatment chemistry will find you
Copper-based preservatives eat zinc. More copper, faster. Wet timber at installation, faster still.
On heavily treated stock and on timber that goes down wet, a thin flake coating is outside its range and no coating weight rescues it. That's hot dip galvanizing or stainless, and it's worth saying out loud to a customer before the deck gets built rather than after his boards have gone black.
I've had that conversation twice this year. Both times the timber was already on site. Both times the answer was no.
Cut ends and field-drilled holes are the same conversation. Touch-up bottles exist, they work reasonably well on a cut end, and almost no crew carries one.
Numbers I'd write on the box for a crew
Pilot 5.5 mm for an M8 in dense hardwood. Skip it and you'll either snap the screw or split the joist, and it happens at the transition under the head rather than in the thread, which is why people blame the screw.
Edge distance three diameters, so 24 mm centre to edge on an M8. End distance closer to seven diameters where the screw is in tension. Those two numbers are what keeps a joist end from tearing out at the worst possible moment.
Joist spacing 400 mm for 25 mm boards, 600 for heavier sections. Clamp before you drive - a screw closing a 3 mm gap is a clamp, and it spends most of its embedment doing that instead of holding the board.
I pulled screws out of a deck two seasons old last year, every head sitting 3 mm below the surface, boards already loose, and the coating was completely intact. Nothing wrong with the fastener. The washer was too small and the driver had no clutch.
Where it fails, and it isn't the head
Not at the head. Not in the thread. It fails at the interface between board and joist, where water sits longest and where installation scraped the coating off.
Second place is the cut end of a field-cut screw, which has no coating at all by definition.
That's the honest limit of a ten micron system, and it's worth stating plainly rather than burying in a data sheet: zinc flake is a good answer for a coastal deck that isn't directly on the water, and a poor one for a deck built from wet, heavily treated timber that gets dragged into place with an impact driver.
What to ask for
Structural or decking, in writing. Board thickness and joist species, which set the length. Exposure and treatment type, which set the coating. Coating weight in g/m² instead of a trademark. And the code report number, because that's the only line on the sheet that tells you somebody tested the thing rather than measured it.
Then ask what happens at a cut end. It's a small question and the answer divides the suppliers who have thought about decks from the ones who are moving boxes.
Hot Tags: dacromet timber screws, structural timber screws, timber screws m8x80, timber screws for decking, decking screws, structural wood screws, dacromet coating