The question was about salt spray
An Australian buyer sent me a drawing with black phosphated written on it and asked how many hours the coating would take, and I said twenty four, and there was a silence on the line that I have learned to recognize as a man deciding whether to be annoyed.
Ninety six, he said. We need ninety six, because the cartons sit on site for three months before they get opened, and if the screws come out of the box with rust on them the fixers will not use them and I will be sending a truck back.
He was right about the three months. He was wrong about what would save him, and it took me two more emails and one very expensive mistake on somebody else's order to work out which part of his reasoning was sound.
Twenty four hours is not a number
A black phosphate on a drywall screw is a light coating, somewhere between one and three grams per square metre, and at that weight it will take twenty four hours of neutral salt spray before red rust appears on about five percent of the surface, which is the figure most of the Chinese mills will quote you and it is honest.
Push the film to six grams and you can get to forty eight, and past that you are not making a drywall screw any more, you are making a screw that costs twice as much and still rusts in a wet season, because phosphate is porous and porosity is the whole trick of the process and porosity is also why it fails.
I have never seen a phosphated drywall screw pass ninety six hours without a topcoat, and any supplier who tells you his does is either talking about white rust or about a different product.
What the coating is doing in the recess
Here is the part that no drawing ever mentions. A phosphate crystal layer has a roughness at the micron scale, and that roughness sits inside the cross recess on the underside of the head and on the flanks of the drive, and it raises the friction between the bit and the recess just enough that the bit grips instead of climbing.
A bright zinc plated screw is slick in the recess by comparison, and on a ceiling where the operator is working overhead with one hand and cannot see the head, the difference between a bit that grips and a bit that climbs is the difference between a screw that goes in and a screw that has to be cut out with a knife.
That is why the black phosphate is on the drawing in the first place, and it has nothing to do with the salt spray figure that the buyer asked me about, and both of us were talking about the same three words on the same line.
Where his screws were sitting for three months
A carton of drywall screws on a site does not sit in the weather. It sits in a container, then in a site hut, then on a pallet under a sheet of polythene with a corner folded back, and the humidity in that stack cycles twice a day and condenses on the coldest surface in the box, which is the steel.
The bottom carton is the one that rusts. Not the top, not the middle, because water runs down and sits and the bottom of a carton is a flat surface with no drainage, and I have opened pallets where the first four cartons were perfect and the fifth was a solid block of paper and rust.
So his ninety six hours was aimed at the wrong thing. He did not need a better coating, he needed a pallet that did not stand in water for a season, and I told him that, and he said the site is the site.
What I quoted and why it was still right
I quoted black phosphate at three grams, because that is the coating his drawing asked for and because at three grams the recess grips and the screw drives the way his fixers expect, and I put the salt spray figure in the email in hours rather than in a word like good.
Then I did the thing that actually solved his problem, which was to change the packing. Four cartons to a heat sealed bag with a desiccant sachet instead of thirty six loose in a box. Two fen a carton. That was the whole cost. It came to less than the freight on the pallet I had already priced for the replacement, and it was the only thing in the entire transaction that made any difference to whether those screws arrived black or arrived orange, and the trucks stopped coming back.
He never asked me about salt spray again. The next drawing he sent had black phosphated on it and a note underneath saying bagged, and I knew exactly which of us had learned what.
The line I want on the drawing
If you are writing a phosphate spec for a drywall screw, do not write black phosphated and stop, because that phrase covers a film from one gram to eight and every one of them will be called the same thing by a mill that wants the order.
Write the film weight in grams per square metre and write the test and the hours you will accept, and write whether the parts are oiled, and then write how they are packed, because on a site the packing decides more of the outcome than the coating does.
The recess grip nobody specifies. It arrives with the phosphate whether you asked for it or not, and it is the reason a bugle head black phosphated sheetrock screws at #6x1-1/4 is the default on a ceiling grid in a dry building, and it is also the reason I no longer try to talk a customer out of it when he asks for the coating for the wrong reason.
Hot Tags: black phosphated sheetrock screws, #6x1-1/4 sheetrock screws, bugle head drywall screws, ceiling grid screws, phosphate coating weight, phillips bit cam out